Why does the screw rod have grinding cracks after intermediate frequency quenching?
Currently, largescrew rodUsually use medium frequency induction hardening. In production, it often happens that the hardened (tempered) screw is screwed into the thread and checked by magnetic inspection. The axial direction is often found to appear on the arc of the thread raceway. In the process of thread grinding, the naked eye can even find cracks or mesh cracks, resulting in the screw being scrapped. This not only causes direct economic losses to the enterprise, but also brings greater pressure to the production of the enterprise due to various factors that cause the problem.

1.Bad raw materials
The main performance isCCr15Unqualified annealing structure of the network carbide of the material (containing lamellar pearlite). Through the analysis of the non-uniformity and microstructure of the crack line stem carbide, the unqualified wire with mesh carbonization or spheroidization annealing tissue accounts for about the total number.40%。
The inhomogeneity of the carbides leads to uneven distribution of the surface hardness and internal stress after induction hardening of the surface of the lead screw. The internal stress is also concentrated in the part where the carbides are more concentrated. When grinding screws, because the internal stress of each part is greater than the yield strength of the material, grinding cracks will appear. The presence of lamellar pearlite leads to coarse grains on the surface of the wire rod after induction hardening, thereby reducing the yield strength of the steel. When grinding the screw rod, the internal stress exceeds the yield strength of the material, resulting in grinding cracks.
2The screw rod is not good in the intermediate frequency quenching heat treatment.
Mainly characterized by high quenching temperature or insufficient tempering. Through analysis and statistics, the screw rod that causes the screw rod grinding crack accounts for about the total number.20%-30%。
When the large screw rod is quenched at intermediate frequency, the output power of the intermediate frequency is too high, and the internal fire of the quenching is too slow, which may cause the screw rod to be quenched at high temperature and the quenching speed of the screw rod is too slow This may cause the screw to quench. High. The coarse martensitic structure reduces the toughness of the steel. In the screw grinding process, the internal stress is greater than the yield strength of the steel, resulting in grinding cracks.
After quenching, the chilled layer is deeper, the internal stress (including thermal stress and structural transformation stress) is large, the tempering is insufficient (low tempering humidity or short tempering time), and the internal The stress formed during the quenching of the screw is removed. After the quenching and tempering of the screw rod, the residual internal stress and the grinding stress generated during the grinding process will be superimposed. When the superimposed stress is greater than the yield strength of steel, cracks will form on the screw surface.